S 101 |
C3 Cr28 Ni4 |
HRc48-54. Resistance to wear, gas corrosion and oxidation. Hardfacing of bucket tooth and case pump. |
|
S 111 |
C1 Cr29 W5 |
HRc38-47. Resistance to wear and corrosion at high-temperature. Hardfacing of high temperature and pressure valve. |
ECoCr-A |
|
S 112 |
C1.5 Cr29 W8 |
HRc45-50. Resistance to wear and corrosion at high-temperature. Hardfacing of valve and hot-rolling pass. |
ECoCr-B |
|
S 113 |
C2.5 Cr30 W17 |
HRc≥55. Wear and heat resistance at high temperature, bad shock resistance. Hardfacing of screw charging carriage. |
||
S 114 |
C2.5 Cr30 W12 |
HRc≥53. Wear and heat resistance at high temperature, bad shock resistance. Hardfacing of three-cone bit. |
ECoCr-C |
|
Copper alloys
銅
合
金 |
S 201 |
Sn1 Si0.3Mn0.3 |
Good mechanical properties and crack resistance. Gas welding and argon arc welding of red copper. |
ERCu |
S 211 |
Si3 Mn1 |
Good mechanical properties. Argon arc welding of copper alloys and MIG brazing of steel. |
ERCuSi-Al |
|
S 212 |
Sn5 Cu Rem. |
Wear resistance. Argon arc welding of copper alloys and surfacing of steel. |
ERCuSn-A |
|
S 213 |
Sn8 Cu Rem. |
Wear resistance. Argon arc welding of copper alloys and surfacing of steel. |
ERCuSn-C |
|
S 214 |
Al7.5 Cu Rem. |
Wear and corrosion resistance. Argon arc welding of copper alloys and surfacing of steel. |
ERCuAl-A1 |
|
S 215 |
Al9 Cu Rem. |
Wear and corrosion resistance. Argon arc welding of copper alloys and surfacing of steel. |
ERCuAl-A2 |
|
S 221 |
Cu60 Sn1 Si0.3 |
Melting point is about 890℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. |
||
S 221F |
Cu60 Sn1 Si 0.3 |
S221 welding rod coated with flux. |
||
S 222 |
Cu58Sn0.9Si0.1 |
Melting point is about 880℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. |
RBCuZn-C |
|
S 222F |
Cu58Sn0.9Si0.1 |
S222 welding rod coated with flux. |
RBCuZn-C |
|
S 223 |
Cu59 Sn0.6 |
Melting point is about 900℃. Braze welding of copper, steel and cast iron. |
RBCuZn-A |
|
S 224 |
Cu62 Si0.5 |
Melting point is about 905℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. |
||
Copper 銅 合 金 |
S 225 |
Cu48 Ni10 |
Melting point is about 935℃ and high strength. Braze welding of steel, nickel and carbide alloys. |
RBCuZn-D |
S 225F |
Cu48 Ni10 |
S225 welding rod coated with flux. |
RBCuZn-D |
|
S 226 |
Cu60 Sn0.3 |
Melting point is about 900℃. Gas welding of brass, also braze welding of copper, steel and cast iron. |
||
S 227 |
Cu58Sn0.9Ni0.5 |
Melting point is about 880℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. |
RBCuZn-B |
|
S 229 |
Cu55 Ni6 Mn4 |
Melting point is about 920℃, high strength. Braze welding of steel, nickel and hard carbide. |
||
Aluminum alloys 鋁 合 金 |
S 301 |
Al≥99.5 |
Good ductility and corrosion resistance. Gas welding and argon arc welding of pure aluminum. |
ER1100 |
S 311 |
Si5 Al Rem. |
Corrosion resistance, wide range of usage. Gas welding and argon arc welding of aluminum alloys other than high magnesium alloys. |
ER4043 |
|
S 321 |
Mn1.3 Al Rem. |
Good corrosion resistance, weldability and ductility. Gas welding and argon arc welding of aluminum alloys. |
||
S 331 |
Mg5 Mn0.4 |
Corrosion resistance and high strength. Argon arc welding of aluminum alloys. |
ER5183 |